AWS E7015-A1 Heat-Resistant Steel Electrode R107 Yakaderera Hydrogen Welding Tsvimbo Electrode

Tsanangudzo Pfupi

R107 (AWS E7015-A1) is pearlitic heat-resistant steel electrode ine low-hydrogen sodium coating ine 0.5% Mo.


Product Detail

Product Tags

Molybdenum uye Chromium Molybdenum Heat Resistant SimbiWeldingElectrode

R107                                                     

GB/T E5015-A1

AWS A5.5 E7015-A1

Tsanangudzo: R107 is pearlitic heat-resistant steel electrode ine yakaderera-hydrogen sodium coating ine 0.5% Mo. Shandisa DCEP (yakananga ikozvino electrode yakanaka) uye inogona kusungirirwa munzvimbo dzese. Iyo weldment inofanira kunge isati yatanga kupisa kusvika 90 ~ 110 ℃ isati yave welding. .

Chikumbiro: Inoshandiswa pakushivirira pombi dzebhailer ine tembiricha yekushanda iri pasi pe510 ° C (senge 15Mo, zvichingodaro), uye inogona zvakare kushandiswa kukwenenzvera general low-alloy high-simba simbi.

 

Kemikari yakagadzirwa nesimbi weld (%):

C

Mn

Si

Mo

S

P

≤0.12

0.50~ 0.90

≤0.50

0.40 ~ 0.65

≤0.030

≤0.030

 

Mechanical zvimiro zve weld simbi:

Test chinhu

Kusimba simba

Mpa

Goho simba

Mpa

Elongation

%

Impact value (J)

Normal Temp.

Guaranteed

≥490

≥390

≥22

≥47

 

Diffusion hydrogen zvemukati mesimbi yakaiswa: ≤6.0mL/100g (glycerin nzira)

X-ray kuongorora: Ini giredhi

 

Yazvino inokurudzirwa:

Tsvimbo dhayamita

(mm)

2.0

2.5

3.2

4.0

5.0

WeldingCurrent

(A)

40 ~ 70

60 ~ 90

90 ~ 120

140 ~ 180

170 ~ 210

 

Cherechedza:

1. Iyo electrode inofanira kubikwa kweawa imwe pa 350 ℃ isati yaitwa welding;

2. Zvinokosha kuchenesa ngura, chikero chemafuta, mvura, uye tsvina pazvikamu zvewelding tisati tasveta.