AWS E7018 Welding tsvimbo J506Fe Iron Powder Yakaderera Hydrogen Potassium Electrode

Tsanangudzo Pfupi

J506Fe (AWS E7018) isimbi yehupfu yakaderera hydrogen potassium electrode.Inoshandiswa pane ese AC uye DC munzvimbo dzese.


Product Detail

Product Tags

Carbon Steel Welding Electrode

J506Fe                                                  

GB/T E5018

AWS A5.1 E7018

Tsanangudzo: J506Fe isimbi yehupfu yakaderera hydrogen potassium electrode.Inoshandiswa pane ese AC uye DC munzvimbo dzese.Sezvo iyo yekuputira iine upfu hwesimbi, ine welding inoshanda zvakanyanya uye inogona kuderedza welding layer.

Chikumbiro: Inoshandiswa kugadzira kabhoni simbi uye yakaderera alloy simbi yegiredhi resimba rinoenderana, senge Q345, nezvimwe.

 

Kemikari yakagadzirwa nesimbi weld (%):

C

Mn

Si

S

P

≤0.12

≤1.60

≤0.75

≤0.030

≤0.035

 

Mechanical zvimiro zve weld simbi:

Test chinhu

Kusimba simba

Mpa

Goho simba

Mpa

Elongation

%

Impact value (J)

(-30℃)

Guaranteed

≥490

≥400

≥22

≥27

Tested

520 ~ 580

≥410

24 ~ 30

50 ~ 180

 

Diffusion hydrogen zvemukati mesimbi yakaiswa: ≤8.0mL/100g (glycerin nzira)

X-ray kuongorora: Ini giredhi

 

Yazvino inokurudzirwa:

Tsvimbo dhayamita

(mm)

2.5

3.2

4.0

5.0

5.8

Welding ikozvino

(A)

90 ~ 120

120 ~ 150

170 ~ 200

210 ~ 250

240 ~ 310

 

Cherechedza:

1. Iyo electrode inofanira kubikwa kweawa imwe pa 350 ℃ isati yaitwa welding;

2. Zvinokosha kuchenesa ngura, chikero chemafuta, mvura, netsvina pazvikamu zvinokandwa musati maveld;

3. Shandisa pfupi arc oparesheni kana welding.Iyo yakamanikana welding track yakakodzera.;

4. Unganidza electrode kune danda rakanaka paunenge uchishanda paDC.

 

Wenzhou Tianyu Electronic Co., Ltd. yakavambwa muna 2000. Tave mushishi mukugadzira maelectrode ewelding, welding rods, uye welding consumables kwemakore anopfuura makumi maviri.

Zvigadzirwa zvedu zvikuru zvinosanganisira Stainless steel welding electrodes, carbon steel welding electrodes, low alloy welding electrodes, surfacing welding electrodes, nickel & cobalt alloy welding electrodes, mild steel & low alloy welding wires, Stainless steel welding wires, gas-shielded flux cored wires, aluminium welding waya, yakanyura arc welding.waya, nickel & cobalt alloy welding waya, ndarira welding waya, TIG & MIG welding waya, tungsten electrodes, carbon gouging electrodes, uye zvimwe welding accessories & consumables.

 


  • Zvakapfuura:
  • Zvinotevera: