AWS ECuSi CopperAlloy Electrode Coated Electrodes T207 Arc Copper Stick Welding Rods

Tsananguro pfupi:

T207 (AWS ECuSi ) ielectrode yemhangura yemhangura ine silicon bronze core uye low hydrogen sodium coating.


Ruzivo rweChigadzirwa

Matagi eChigadzirwa

Electrode yeWelding yeCopper neCopper Alloy

T207                                                     

GB/T ECuSi-B

AWS A5.6 ECuSi

 

Tsananguro: T207 ielectrode yemhangura yemhangura ine silicon bronze core uye low hydrogen sodium coating. Shandisa DCEP (direct current electrode positive) ine hunhu hwakanaka hwemakanika. Inodzivirira ngura zvakanaka kune inorganic acids kunze kwe nitric acid, akawanda organic acids nemvura yegungwa.

 

Mashandisirwo: Yakakodzera kusanganisa mhangura, silicon bronze nendarira, kusanganisa pamusoro pemapeipi emakemikari, nezvimwewo.

 

Kuumbwa kwemakemikari esimbi ye weld (%):

Cu

Si

Mn

Pb

Al+Ni+Zn

>92.0

2.5 ~ 4.0

≤3.0

≤0.02

≤0.50

 

 

Hunhu hwesimbi ye weld:

试验项目

Chinhu chekuyedza

抗拉强度

Simba rekusimba

Mpa

延伸率

Kureba

%

保证值

Yakavimbiswa

≥270

≥20

 

 

Inokurudzirwa yemagetsi:

Dhayamita yetsvimbo

(mm)

3.2

4.0

5.0

Welding Current

(A)

90 ~ 130

110 ~ 160

150 ~ 200

 

Cherechedza:

Zvekungwaririra:

1. Electrode inofanira kubikwa pa300°C kweawa imwe kusvika maviri isati yaiswa;

2. Hunyoro, mafuta, maokisijeni nezvimwe tsvina zviri pamusoro pe weldment zvinofanira kubviswa zvisati zvabatanidzwa.

3. Pakusanganisa silicon bronze kana welding pamusoro pesimbi, hapana kudziya kunodiwa. Tembiricha yekupisa yekusanganisa mhangura yakachena inenge 450°C, uye tembiricha yekupisa yekusanganisa mhangura inenge 300°C;

4. Kusonwa kwesimbi kupfupi kunofanira kushandiswa panguva yekusonwa. Panguva yekusonwa kwesimbi kunofanira kunge kwakabatana nesimbi dzakawanda.

zvabviswa zvachose; mushure mekusunga, gadzira weld nehammer yakatsetseka kuti unatsiridze tsanga, kubvisa kushushikana, uye kuvandudza kusimba uye plasticity yeweld.